Your current position: Home >> Coating defects caused by improper use of atomic ash

Coating defects caused by improper use of atomic ash


 Coating defects caused by improper use of atomic ash

 
In the automobile coating process, the top coat is the last process of Z. with the continuous development of the automobile industry, many manufacturers now use baking paint. If there is a problem after finishing, it is Z troublesome. The following atomic ash manufacturers will make a brief introduction according to the problems in production.
 
1. The top coat foams after baking.
 
Scrape off the bubbles after the bubbles of the top coat and see which layer the bubbles are on. If the bubbles appear in the primer layer, the atomic ash is well combined with the primer, and the substrate treatment may not be in place; After blowing off the bubbles, it is found that there is a layer of primer on the atomic ash and the substrate. Then it may be that the primer is too thick or the primer is not dry enough.
 
2. Pinholes and depressions appear after baking the finish paint.
 
First of all, consider whether the pinhole has its own quality. Secondly, if pinholes appear when the quality of atomic ash is qualified, it is generally because the atomic ash coating and grinding technology is poor and the sand holes are not handled well. In addition, during the coating and scraping process, if the coating and scraping tool is improperly selected, it will also cause pinholes.
 
3. "Prickle" after baking the finish coat.
 
First, the climate is too humid and the water absorption of the atomic ash is too large. The polished atomic ash adsorbs a considerable amount of water. The topcoat is sprayed before the water volatilizes. A small amount of water is sealed under the paint film. Once heated, the water volume expands sharply and breaks through the paint film to form a "prickly heat". Second, the water absorption of atomic ash is qualified. After being dried by hot air, spray the top coat, and there is "prickly heat" after baking. Then it is possible that after spraying the top coat, the solvent enters the drying room before it volatilizes fully. In this way, because the surface of the top coat is closed soon, the residual solvent has to break through the paint film to form "prickly heat". Of course, it may also be the quality problem of the topcoat, or the mismatch between the polarity of the solvent and the topcoat


Prev What are the types of atomic ash
NextSteps for scraping atomic ash

Copyright © 2020 Changxing Baodi Environmental Protection Technology Co., Ltd all reserved Web Admin --> >>

浙公網安備 33052202000243號?浙ICP備17019658號

主站蜘蛛池模板: 赞皇县| 小金县| 涿州市| 山丹县| 咸宁市| 搜索| 滦南县| 营口市| 容城县| 海淀区| 谢通门县| 镇康县| 荥阳市| 霍城县| 五莲县| 自治县| 长白| 浮梁县| 奇台县| 安溪县| 福建省| 宁远县| 噶尔县| 隆尧县| 土默特左旗| 凉城县| 高邑县| 墨脱县| 清远市| 象山县| 延边| 虹口区| 鄂伦春自治旗| 嘉善县| 罗甸县| 大化| 石城县| 博罗县| 河南省| 怀远县| 图片|